P22 is the 2.25% chromium, 1% molybdenum workhorse of high-temperature piping - the grade behind most power station headers, reheater links and refinery furnace transfer lines designed up to roughly 550 degrees C. It carries about twice the chromium of P11 and double the molybdenum, which buys real creep strength in exchange for stricter welding and heat treatment discipline. This page is the buyer-level view: chemistry, where P22 beats its neighbors, and the fabrication details that decide whether an order passes inspection the first time.

Chemistry and Strength at Temperature
| Item | A335 P22 requirement |
|---|---|
| Carbon | 0.05-0.15% |
| Chromium | 1.90-2.60% |
| Molybdenum | 0.87-1.13% |
| Tensile strength, min | 415 MPa |
| Yield strength, min | 205 MPa |
| Required condition | Normalized and tempered |
Table note: values per ASTM A335/A335M. Design allowables at temperature are set by the construction code, not the pipe standard.
The practical meaning of that chemistry shows up above 480 degrees C, where P11 has started to lose creep margin and carbon steel is not in the conversation at all. P22 holds useful stress up to about 540-550 degrees C continuously, and its oxidation behavior stays clean enough that bore condition after years of steam service remains a non-issue. It is also the base chemistry for the famous 2.25Cr-1Mo vessel steel - the same alloy family as ASTM A387 Grade 22 alloy steel plate - so piping and vessel plate on one project often share heat-treatment thinking.
P22 vs P11 vs P91: Choosing Between Neighbors
| Question | P11 | P22 | P91 |
|---|---|---|---|
| Design temperature band | to about 500 C | to about 550 C | to about 600 C |
| Welding difficulty | Moderate | Moderate, preheat advised | High, PWHT mandatory |
| Relative pipe cost | 1.0 (reference) | about 1.2-1.4 | about 2 or more |
| Typical fail mode if misapplied | Creep thinning above band | Creep above band | Weld zone cracking if PWHT skipped |
Table note: relative costs vary with heat availability and size; use them for first-pass screening only.
The selection logic in one line: buy P11 until the temperature or the design life pushes you out of it, buy P91 when the temperature pushes you out of P22 or when wall thickness with P22 becomes unbuildable, and buy P22 for everything in the broad middle where it is the cheapest grade that survives. The expensive mistake is the reverse - specifying P91 where P22 would do, because P91's welding and PWHT regime costs the fabricator more than the pipe saving is worth.
Fabrication: Welding and PWHT
P22 welding is well understood: matching Cr-Mo filler, preheat typically 150 to 200 degrees C depending on thickness, and post-weld heat treatment around 650 to 700 degrees C for most code work. The failures we see are not exotic - they are skipped or under-soaked PWHT on thick wall joints, and hardness surveys that were promised but never taken. If your fabricator has P11 experience, P22 is a small step; if the team has never run alloy PWHT, budget for a procedure qualification before the first production weld.
Ordering Details That Get Missed
Three items decide most P22 orders. Impact testing: refinery and power specs often call for Charpy at a stated temperature, which must be booked with the heat, not added after. Elevated temperature tensile: some turbine and header specs want yield at 450 or 500 degrees C on the certificate. And size honesty: large OD P22 (above 457 mm) runs long production queues because the piercing capacity for heavy alloy is limited - if your schedule is tight, read our lead time note for steel pipe from China and plan the order around the mill run. For the standard's overall picture, including sizes and the test menu, start from the ASTM A335 alloy steel pipe overview.
Is P22 the same as T22 or 10CrMo9-10?
Same 2.25Cr-1Mo chemistry family. P22 is pipe (A335), T22 is tube (A213), 10CrMo9-10 is the German EN designation with its own standard and slightly different test rules. Equivalences are close but not paper-identical - check the datasheet before substituting.
What PWHT temperature does P22 need after welding?
Typically 650 to 700 degrees C depending on wall thickness and the construction code. The certificate from the mill shows the pipe's own normalizing and tempering temperatures; the field joints must land in the same condition, which is what a hardness survey verifies.
Can P22 be used in hydrogen service?
Yes, within the Nelson curve limits for 2.25Cr-1Mo - it is a standard refinery hydrogen grade. Confirm operating temperature and hydrogen partial pressure against the current curve revision at design stage.
How do I verify a P22 offer is genuine?
Ask for an MTC from a recent heat and check the actual normalizing and tempering temperatures plus heat traceability. Offers without treatment temperatures on the certificate are the ones that fail third-party inspection.
Hot Tags: p22 alloy steel pipe, astm a335 p22, a335 gr p22 pipe, 2.25Cr 1Mo pipe, p22 seamless pipe China supplier, p22 pipe price